Friday, November 4, 2011

6g trouble

I have a weld test coming up its on 3/4 stainless coupling at the 6g postion . Im having trouble with the botttom of the weld dripping i call it seagul poo . I cant go.any lower temp because the specs for the test has a range of 55 amps to 75 amps any help
--------------------------------

have you tried using a slight weaving motion or a series of small loops with the rod?

stainless stick wants to drip and sag but you have to fight against it.

try using about 70 amps and a tight arc making a series of loops.

you have to be able to hold a tight enough arc to keep the weld metal pushed flat, while at the same time, you have to get moving and not let the heat build up too much.

No comments: